Document Type : Systematic Review

Authors

1 Dept. of Operative Dentistry, Dental Materials Research Center, Dental Research Institute, School of Dentistry, Isfahan University of Medical Sciences, Isfahan, Iran.

2 Dept. of Endodontics, Dental Research Center, Dental Research Institute, School of Dentistry, Isfahan University of Medical Sciences, Isfahan, Iran.

3 Dept. of Endodontics, School of Dentistry, Rafsanajn University of Medical Sciences, Rafsanjan, Iran

4 Dept. of Operative Dentistry, School of Dentistry, Rafsanjan University of Medical Sciences, Rafsanjan, Iran.

10.30476/dentjods.2023.97057.1986

Abstract

Statement of the Problem: Immediate dentin sealing (IDS) was introduced to overcome the disadvantages of delayed dentin sealing like pollution of dentin tubules, microleakage, and bond strength destruction over time. The effect of IDS on the bond strength of indirect restorations is still debatable.
Purpose: This study was conducted to determine the effect of IDS on the bond strength of ceramic restorations to dentin.
Materials and Method: In this systematic review and meta-analysis, the study protocol was registered on the PROSPERO database under the registration number CRD420202014 27. MEDLINE (PubMed), Web of Science, Scopus, and ProQuest databases were searched until January 2021 and updated in January 2022. Worldcat.org and Opengrey.eu, ProQuest dissertation and thesis, and Google Scholar were searched to explore the grey literature. The in vitro studies evaluating the bond strength of ceramic restoration to dentin with and without IDS were included. Seven criteria were assessed to evaluate the risk of bias in the study. Statistical analyses were conducted using RevMan 5.3. The inverse variance method was used to determine the mean difference of micro-tensile bond strength (µTBS) and shear bond strength (SBS).
Results: A total of 10 studies (20 datasets) were included in the meta-analysis. Regarding the µTBS analysis, IDS had a significantly higher bond strength than Delayed Dentin Sealing (DDS) (MD:1.16, 95%CI:0.28_2.03, I2=0%). However, no significant difference was found between them in the SBS analysis (MD:0.25, 95%CI: -0.56-1.06, I2=96%). All studies were categorized to have a moderate or high risk of bias.
Conclusion: Most in vitro evidence showed favorable results for the effect of IDS on the bond strength and durability of indirect restorations. The adhesive system and the type of ceramic and its treatment before cementation are determining factors. Due to the heterogeneity of the outcomes and studies with a moderate/high risk of bias, the quality of the evidence was low.

Keywords

Introduction

The use of tooth-colored materials to restore decayed teeth, particularly in the posterior areas of the mouth, is important for many patients [ 1 ]. The direct use of composite resins for the reconstruction of teeth where gross tooth destruction has occurred and requires a vast reconstruction, especially the proximal contours, is too challenging and sometimes even impossible [ 2 ]. In these situations, the use of indirect restorations allows accurate reconstruction of the tooth crown and has better contours, wear resistance, and mechanical strength than the direct ones [ 2 - 3 ].

However, the disadvantages of indirect restorations such as tooth sensitivity that occasionally occurs in vital teeth, bond strength reduction over time, deboning, secondary caries, and fractures should be noted since they compromise the survival rate [ 4 - 5 ]. Hence, the improvement of bond strength is an important factor to enhance the success rate and fracture resistance, decrease microleakage, and increase the overall survival rate [ 6 ].

The conventional method used for the cementation of indirect restoration is delayed dentin sealing (DDS), which briefly includes the application of adhesive resins just before cementation [ 7 - 10 ]. Resin coating technique was introduced by Pashley et al. [ 11 ] in the 1990s to improve the properties of indirect restorations and to reduce tooth sensitivity. Later in 2005, Magne et al. [ 12 ] introduced immediate dentin sealing (IDS) based on the resin coating technique. This procedure involves the sealing of freshly cut dentin tubules filled with an adhesive resin alone or in combination with a low-viscosity resin prior to (digital or analog) impression-taking [ 12 ]. The use of IDS has been effective in improving the bond strength of indirect restorations [ 13 - 16 ]; however, some studies have indicated no priority for DDS regarding the long-term bond strength [ 17 ].

Considering the lack of consistency among the results of studies on the effect of IDS on the bond strength of indirect restorations and the lack of a comprehensive review in this field, this systematic review and meta-analysis aimed to evaluate the effect of IDS on the bond strength of ceramic restorations.

Materials and Method

Protocol and registration

The study protocol was registered on the PROSPERO database under the registration number CRD4202020-14 27. The Preferred Reporting Items for Systematic Reviews and Meta-Analyses (PRISMA) checklist was used to report this systematic review [ 18 ].

Forming the question

The research question, based on the patient, intervention comparison, outcome, study (PICOS) framework, was “Does IDS improve the bond strength of ceramic restorations to dentin in comparison with IDS in experimental studies?”

The PICOS framework was set as P: human teeth with ceramic restoration, I: IDS, C: DDS, O: effect on micro-tensile bond strength (µTBS) or shear bond strength (SBS), and S: experimental studies.

Study eligibility criteria

The inclusion criteria were all experimental studies that evaluated the SBS or µTBS of ceramic restorations to dentin using IDS. The exclusion criteria were studies that evaluated properties other than the bond strength of ceramic restorations to dentin, studies that evaluated the bond strength of other types of restorative materials, clinical trials, all types of reviews, case reports, or case series.

Information sources and search strategy

The keywords in the search strategy were defined based on the PICOS framework. An unlimited literature search was undertaken on the MEDLINE (PubMed), Web of Science, Scopus, and ProQuest databases. Worldcat.org and Opengrey.eu, ProQuest dissertation and thesis, and the first 100 results in Google Scholar were searched to explore the grey literature until January 2021 and updated in January 2022. A manual search was performed to explore the reference lists of all primary studies for the additional relevant publications linked to each primary study on the PubMed database. The search strategies in the four main databases are listed in Table 1. The search was restricted to English language.

Database Search line Number of retrieved records
MEDLINE (PubMed) (“immediate dentin sealing” OR “dentin sealing” OR “resin coating”) AND (“bond strength” OR “Shear bond” OR “tensile bond”) 78
Scopus TITLE-ABS-KEY ((“bond strength” OR “Shear bond” OR “tensile bond”) AND (“immediate dentin sealing” OR “dentin sealing” OR “resin coating”)) 94
Web of Science TS= (((“immediate dentin sealing” OR “dentin sealing” OR “resin coating”)) AND (“bond strength” OR “Shear bond” OR “tensile bond”)) 90
ProQuest (“immediate dentin sealing” OR “dentin sealing” OR “resin coating”) AND (“bond strength” OR “Shear bond” OR “tensile bond”) 309
Table 1.Search strategy of the databases from their foundation until January 2021 and updated January 2022

Study selection and data collection

After the removal of the duplicate studies, the records were selected by titles and abstracts. In the next stage, full-text articles were screened for including records meeting the inclusion criteria. The study selection was done by two researchers independently, and any disagreement was resolved through discussion with other reviewers. Google sheets software was used as a customized extraction form to extract relevant data. The extraction form consisted of the first author’s name, year of publication, number of samples, adhesive system for IDS, type of aging protocol (mechanical or thermal or none), type of luting agent, type of ceramic, porcelain treatment before cementation, and main out come. Data were extracted by two reviewers independently, and any disagreement was resolved via discussion with other reviewers. In case of missing data, an email was sent to the corresponding author. If the authors did not answer up to one month twice, the record was excluded.

Quality assessment

The quality assessment of each included study was independently assessed by two reviewers using the checklist of other systematic reviews [ 19 ]. The parameters consisted of (1) randomization of teeth, (2) use of teeth free of caries or restoration, (3) use of materials according to the manufacturer’s instructions, (4) use of teeth with similar dimensions, (5) description of sample size calculation, (6) treatment performed by the same operator, and (7) blinding of the operator of the testing machine. If it was possible to find the information in the article, it received an ‘‘Y’’ (yes) answer and vice versa. Studies that reported one to three items were classified as high risk of bias, four or five items as a medium risk of bias, and six or seven items as a low risk of bias. Any disagreements were resolved through discussion with a third reviewer.

Synthesis of results

The data of each study were fed into RevMan 5.3 (The Cochrane Collaboration, Copenhagen, Denmark). Mean difference (MD) was determined for µTBS and SBS by inverse variance method. For subgroup analysis, studies were divided based on the bonding system used for the IDS, cement type, and ceramic restoration type and ceramic treatment before cementation. Statistical heterogeneity of the treatment effect was assessed using the inconsistency I2 test in which values greater than 75% were considered highly heterogeneous [ 20 ]. The sensitivity analysis was conducted by removing the studies with a high risk of bias.

Results

Study selection

A total of 892 relevant records were extracted from the databases. Figure 1 is a PRISMA flowchart that summarizes the article selection process. After the removal of duplicates, 321 records were evaluated for the titles and abstracts, from which 291 records were excluded. Therefore, 30 records were subjected to full-text evaluation. Of them, 20 studies were excluded. Table 2 shows the records excluded with reasons in the full-text assessment phase. Finally, 10 records [ 4 , 7 - 8 , 13 , 15 - 17 , 21 - 23 ] were used for qualitative and quantitative synthesis. Ten studies were included, of which 4 studies used µTBS test and 6 used SBS test.

Figure 1. Preferred reporting items for systematic reviews and meta-analyses flow diagram of the search processes

Reasons for exclusion References
Evaluation of the effects of IDS on the bond strength of cement to ceramic n=1
Evaluation of the effect of IDS on the bond strength of metal restorations to teeth n=1
Evaluation of the effect of IDS on the bond strength of laboratory or chair side or CAD CAM resin composite to teeth n=17
Not having DDS as a control group n=1
Table 2.Studies excluded with reasons in the full-text asses-sment phase; IDS: immediate dentin sealing, DDS: delayed dentin sealing

Characteristics of the included datasets

As for µTBS test, all datasets used a non-self-adhesive luting system for the ceramic cementation and evaluated the bond strength of silica-based ceramics. Except one dataset, self-etch adhesive systems were used for IDS in other datasets [ 23 ] (Table 3). Regarding SBS test, all studies except one [ 17 ] used non-self-adhesive resin cement and all of the studies evaluated the bond strength of silica-based ceramics to teeth except one [ 13 ] which evaluated the bond strength of non-silica-based ceramics (monolithic zirconia). This study used two different materials for cementation (with Panavia F2 or PermaCem). It is noteworthy that only Panavia results were included for better comparison, the same as other included studies (Table 4). Each study in both categories used a different protocol for porcelain treatment before cementation, e.g. etching by Hydrofluoric acid (HF), Airborne-Particle Abrasion (APA), CoJet (CJ) abrasion, or none. There was a huge variation in the aging protocols in both categories.

Study Adhesive system Sample size per group (N) Type of aging Type of luting agent Type of ceramic Porcelain treatment before cementation IDS/ mean (Mpa) (SD) DDS/ mean (Mpa) (SD)
Ishi et al. [ 21 ] Etch-and-rinse 4 Artificial mechanical Non-self-adhesive Silica-based Airborne Particle Abrasion (APA) 5.1(1.2) 3.5(1.6)
Hayashi et al. [ 16 ] Self-etch 30 Artificial mechanical Non-self-adhesive Silica-based Hydrofluoric acid (HF) 4.9(2.0) 3.8(1.7)
Kitayama* et al. [ 22 ] Self-etch 14 Artificial mechanical Non-self-adhesive Silica-based Airborne Particle Abrasion (APA) 12.97(5.82): N (60/98) (Number of beams, tested/ total) – (0/89)
Kitayama. et al. [ 22 ] Self-etch 14 No Non-self-adhesive Silica-based Airborne Particle Abrasion (APA) 15.17 (5.24): N (49/81) 15.82 (4.22): N (45/78)
Murata**et al. [ 4 ] Self-etch 8 Artificial mechanical Non-self-adhesive Silica-based n/a 5.8(2.3) 4.4(1.5)
IDS: immediate dentin sealing, DDS: delayed dentin sealing, n/a: Not applicable, HF: Hydrofluoric acid, APA: Airborne particle abrasion, CJ: CoJet Superscript letters show different datasets from one study.
* Samples with artificial aging were not included because all samples in the DDS group failed in the pretest.
** Three different IDS applications were used, but just one of them was included in the analysis because this method was more similar to other included studies.
Table 3.Studies that used µTSB
Study Adhesive System Sample size pre group (n) Type of aging Type of luting agent Type of ceramic Porcelain treatment before cementation IDS/ mean (Mpa) (SD) DDS/ mean (Mpa) (SD)
Falkensammer et al. [ 7 ] Self-etch 48 No Non-self-adhesive Silica-based Hydrofluoric acid (HF) 13.7(4.7) 19.5(4.0)
Shakal*et al. [ 8 ] Etch-and-rinse 10 Artificial thermal Non-self-adhesive Silica-based Airborne Particle Abrasion (APA) 7.50(0.78) 8.00(0.31)
Shakal et al. [ 8 ] Etch-and-rinse 10 No Non-self-adhesive Silica-based Airborne Particle Abrasion (APA) 9.42(0.56) 10.06(0.44)
Shakal et al. [ 8 ] Etch-and-rinse 10 Artificial thermal aging Non-self-adhesive Silica-based Hydrofluoric acid (HF) 8.00(0.79) 8.82(0.389)
Shakal et al. [ 8 ] Etch-and-rinse 10 No Non-self-adhesive Silica-based Hydrofluoric acid (HF) 8.14(0.44) 8.86(0.384)
Shakal et al. [ 8 ] Etch-and-rinse 10 Artificial thermal aging Non-self-adhesive Silica-based CoJet (CJ) 7.62(0.49) 8.10(0.22)
Shakal et al. [ 8 ] Etch-and-rinse 10 No Non-self-adhesive Silica-based CoJet (CJ) 8.14(0.44) 10.50(0.41)
Shakal et al. [ 8 ] Etch-and-rinse 10 Artificial thermal aging Non-self-adhesive Silica-based N 4.44(0.52) 4.88(0.544)
Shakal et al. [ 8 ] Etch-and-rinse 10 No Non-self-adhesive Silica-based N 6.00(0.79) 7.52(0.37)
Reboul et al. [ 23 ] Etch-and-rinse 10 No Non-self-adhesive Silica-based Hydrofluoric acid (HF) 15.74 (2.12) 12.07(1.41)
Choi**et al. [ 15 ] Etch-and-rinse 10 Artificial thermal aging Non-self-adhesive Silica base Hydrofluoric acid (HF) 4.11(2.82) 3.14(1.47)
Choi et al. [ 15 ] Self-etch 10 Artificial thermal aging Non-self-adhesive Silica-bases Hydrofluoric acid (HF) 11.18 (4.75) 3.14 (1.47)
Dalby*** et al. [ 17 ] Etch-and-rinse 13=Opti bond FL No Self-adhesive Silica-based Hydrofluoric acid (HF) 10.03 (3.50) 7.17(2.09)
11=single bond 8.24(3.35)
11=DDS
Dalby et al. [ 15 ] Self-etch 8 samples=Go! No Self-adhesive Silica-based Hydrofluoric acid (HF) 6.94 (1.53) 7.17(2.09)
11 samples= one coat bond
11 samples in DDS group 7.21(2.83)
Rigos ****et al. [ 13 ] Etch-and-rinse 15 No Non-self-adhesive Non-silica-based Airborne Particle Abrasion (APA) 39.94 (1.34) 33.40 (1.76)
Rigos et al. [ 13 ] Etch-and-rinse 15 No Non-self-adhesive Non-silica-based CoJet (CJ) 38.68 )1.16) 29.37(2.16)
* According to different porcelain treatment before cementation and aging or non-aging variables included in eight datasets
**,***Each included two datasets according to different adhesive systems.
****Assessed in two data sets according to different porcelain treatment before cementation
Table 4.Studies that used SBS test

Risk of bias in individual studies

Overall, in the µTBS group, all studies were categorized as moderate (1 study; 25%) or high risk of bias (3 studies; 75%). In the SBS group, four (66.6%) and two (33.3%) studies showed a moderate and high risk of bias, respectively. No studies (100%) in each group mentioned sample size calculation and blinding of the operator of the testing machine. Moreover, 100% and 66.6% of studies in the µTBS and SBS groups did not mention the treatment was performed by a single operator. Hence, at least three out of seven items received NO answers for included studies, and none of them was categorized as a low risk of bias (Tables 5 and 6).

Study Tooth randomization Teeth free of caries or restoration Materials used according to the manufacturer’s instructions Teeth with similar dimensions Sample size calculation Treatment performed by a single operator Blinding of the operator of the testing machine Risk of bias
Maeno et al. [ 16 ] N Y Y Y N N N High risk
Kitayama et al.[ 22 ] Y Y Y Y N N N Moderate risk
Maeski et al.[ 4 ] N Y Y Y N N N High risk
Ishi et al.[ 21 ] N Y Y Y N N N High risk
Table 5.Assessment of the risk of bias of µTSB (n = 4)
Study Tooth randomization Teeth free of caries or restoration Materials used According to the manufacturer’s instructions Teeth with similar dimensions Sample size calculation Treatment performed by a single operator Blinding of the operator of the testing machine Risk of bias
Falkensammer et al.[ 7 ] No Yes Yes Yes No No No High risk
Choi et al. [ 15 ] Yes Yes Yes Yes No No No Moderate risk
Dalby et al. [ 17 ] Yes Yes Yes Yes No Yes No Moderate risk
Shakal et al. [ 8 ] Yes Yes Yes N No No No High risk
Reboul et al. [ 23 ] Yes Yes Yes Yes No Yes No Moderate risk
Rigos et al. [ 13 ] Yes Yes Yes Yes No No No Moderate risk
“Y” = “Yes” and shows reported item “N” = “No” and shows not reported item
Table 6.Assessment of the risk of bias of shear bond strength (SBS) (n = 6)

Meta-analysis

The meta-analysis indicated that IDS had no positive effect on the SBS (MD:0.25, 95%CI: -0.56-1.06, I2= 96%) (Figure 2). In subgroup analysis, IDS demonstrated no positive effect on the SBS when silica-based ceramics were used (MD: -0.36, 95%CI: -1.00-0.27, I2=93%). Li-kewise, in subgroup analysis, IDS demonstrated no positive effect on the SBS when non-self-adhesive cements were used as a luting agent (MD: 0.12, 95%CI: -0.73-0.96, I2=97%). The results of the analysis of non-artificial and artificial aging datasets showed no statistically significant difference (MD: -0.12, 95%CI: -1.64-1.40, I2=98% and MD: -0.10, 95% CI: -0.77-0.57, I2=85%), respectively). Although applying etch-and-rinse systems for IDS did not improve the SBS (MD:1.06, 95%CI: 0.36-2.09, I2=98%), the self-etch systems enhanced the SBS (MD:0.66, 95% CI:-6.38-7.69), I2=97%).

The meta-analysis indicated that IDS had a positive effect on the µTBS (MD:1.16, 95%CI:0.28_2.03, I2= 0%) (Figure 3). In subgroup analysis, IDS improved the µTBS after aging or applying self-etch adhesive systems (MD:1.27, 95%CI:0.37-2.18, I2=0% and MD: 1.04, 95%CI: 0.07-2.05, I2=0%, respectively).

Figure 2. Forest plot of the analysis of immediate dentin sealing (IDS) on shear bond strength (SBS) compared to Delayed Dentin Sealing (DDS). Event: shear bond strength (SBS) in Mpa

Figure 3. Forest plot of the analysis of immediate dentin sealing (IDS) on µTBS compared to delayed dentin sealing (DDS). Event: µTBS in Mpa

The results of sensitivity analysis (after eliminating the high-risk studies) in both SBS and µTBS categories showed that MD was significantly higher in DDS than in IDS (MD:4.13 95%CI:078-7.48, I2=96.5% and MD:-0.65 95%CI:-4.17-2.78, I2=NA, respectively), which was different from the main analysis. Hence, the robustness of the analysis was low.

Discussion

IDS was first introduced in 2005 to improve adhesion and restorative adaptation and to protect the pulp vitality [ 24 ]. The primary technique involves the application of an etch-and-rinse adhesive to the dentin surface. After taking the impression in the delivery session, an indirect restoration was applied after sandblasting with a non-self-adhesive cement on the IDS surface, which was conditioned by a brush and pumice [ 12 ]. Since then, different IDS methods with different types of bonding, intaglio surface preparation methods, IDS surface conditioning, and direct and indirect restorations with different materials have been studied, which have shown different results [ 25 - 28 ]. Therefore, the outcome of the present study may help practitioners make better clinical decisions.

The results of the included studies according to the test used for measuring bond strength were assessed in two categories: SBS and µTBS. The present meta-analysis showed that µTBS was higher with IDS than with DDS, and there was no significant difference between the two groups in SBS. The SBS has easy sample preparation and less technical sensitivity, but the samples in µTBS can be highly affected by adverse events such as premature failures and need a larger number of samples [ 25 - 28 ]. Yet, the more uniform stress distribution achieved by the µTBS test than the SBS [ 29 ] is a considerable factor, so the simplicity of the SBS test seems not to be a good reason for choosing this test to evaluate the bond strength [ 30 ].

In case of mechanical or thermal aging of the samples, the µTBS of IDS was higher than that of DDS, but the difference was not significant in the SBS analysis. Thus, the use of IDS may increase the bonding durability. The positive effect of IDS on durability is probably due to the sufficient and effective penetration of the resin into the newly cut dentin collagen fibers of the tooth and the formation of a sufficiently thick hybrid layer compared to DDS. In the absence of dentin sealing, the collagen fibers collapse during impression-taking, and their interfibrillar spaces are reduced for the resin to penetrate [ 31 - 32 ]. On the other hand, in the case of temporary restoration, even despite the use of various surface cleaning methods to remove cement residues (such as air-abrasion), dentin is contaminated with temporary cement and prevents adequate interaction between the adhesive and collagen [ 33 ]. If temporary restoration is not used, or restoration does not have enough sealing, the dentin becomes contaminated, and all these factors interfere with the penetration of the resin and the formation of an effective hybrid layer, which endangers the immediate bond strength of the dentin [ 34 ].

IDS also prevents the denaturation of collagen structure over time by sealing tubules and preserving exposed collagen in the freshly cut dentin and preventing the contamination and activation of proteolytic enzymes [ 35 , 36 ]. Furthermore, this layer acts as a stress reliever and protects the bonding layer against mechanical forces [ 4 ]. Another positive effect is due to the maturation of the adhesive layer (IDS) by the dark curing mechanism and the continuation of polymerization until the cementation is performed. This process reduces the stresses due to the polymerization of the cement and the occlusal forces on the newly created hybrid layer with low strength compared to DDS [ 37 - 38 ]. Since the bond strength decreases over time, according to the results, it may be possible to confirm the results of previous studies about the effect of IDS on increasing the bond durability [ 12 , 16 ].

The bond strength, in terms of the type of adhesive system, indicated that although the SBS of IDS was not higher in the etch-and-rinse system, the µTBS of IDS was higher in the self-etch subgroup. The bonding systems with fillers or functional monomers (creating a chemical bond) in the etch-and-rinse subgroup of the SBS group were used in most studies [ 39 - 41 ], which, if used correctly, create high strength. Thus, IDS can be used with all types of bonding systems to create sufficient film thickness as recommended by Magne et al. [ 42 ]. It can also be as effective as OptiBond FL, which is the gold standard of adhesive materials.

The µTBS and SBS of IDS and DDS groups were the same when different ceramic surface preparation methods were applied before cementing the restoration. However, the bond strength decreased in preparation with silicate, air-abrasion, and hydrofluoric acid, respectively. This result can be due to the dual chemical and mechanical bonding properties of air-abrasion systems with silicate particles and increased surface roughness in air-abrasion compared to hydrofluoric acid [ 8 , 43 - 44 ]. Therefore, surface preparation methods are highly effective in improving the bond strength, and the main purpose of using IDS is not to increase the bond strength.

Despite the numerous advantages mentioned for IDS in studies, this technique is time-consuming and requires more materials and steps. This method has a high technical sensitivity. If the adhesive layer is too thick, the strength of ceramic restorations will decrease due to less space and a large difference in the elastic coefficient of the adhesive layer and restorations, especially ceramic restorations [ 45 - 46 ]. On the other hand, if a very thin adhesive layer (less than 40 microns) is formed, all the thickness of the adhesive turns into an air-inhibited layer and the adhesive does not polymerize, and this method practically loses its clinical effectiveness [ 47 ]. To reduce the interference of temporary restorations and common impression materials, the tooth should be covered with Vaseline after IDS so that the monomers in the temporary restorative resin are not bonded to the adhesive layer [ 24 , 48 ]. Moreover, instead of using temporary cement, mechanical gear should be created with the help of undercuts, embracers, and temporary splints, and the final restoration should be delivered and cemented in the shortest possible time (up to 1 week) [ 49 ]. To eliminate the interference with the impression materials, it is recommended to use digital impression-taking methods, and if impression materials are used, the oxygen-inhibiting layer of the IDS surface should be thoroughly cleaned and removed to prevent complete polymerization of the impression materials [ 50 - 51 ].

Few clinical studies have investigated the effectiveness of this technique. Gresnigt et al. [ 52 ] reported that IDS increased the survival rate of restorations if more than 50% of dentin was exposed. However, Van den Breemer et al. [ 53 ] showed IDS was not superior in the survival rate and success of restorations. The heterogeneity of the population in terms of oral health and different experiences of clinicians may be the reasons for these contradictions [ 53 ].

Due to the lack of clinical trials, the present study was performed on in vitro studies. The high heterogeneity of the SBS studies indicates the diversity of the materials and methods used. The quality of most studies in both groups was categorized as moderate to high risk of bias. It should be noted among a seven-item criterion proposed, three criteria of sample size calculation, the blinding of the operator of the testing machine, and performing the treatment by one operator were not mentioned in most studies. Thus, several variables in the design of laboratory studies were not controlled or reported, which might be due to the lack of an accepted guideline. By excluding the high risk of bias studies, the outcome was different from the main outcome for each group, indicating low consistency. Most of the included studies evaluated the SBS. However, owing to the advantages of µTBS, it is suggested for the bond strength evaluation in this area. More studies with a better design are needed to achieve a definitive result.

Conclusion

Most in vitro evidence showed the favorable impact of IDS on the bond strength and durability of indirect restorations. The use of any standard etch-and-rinse adhesive system or self-etching system is effective to obtain the desired results with IDS. The use of pre-treatment ceramic surface preparation methods reduces the difference in the IDS impact. However, the results of the in vitro studies should be used in clinical settings with caution. In addition, the included studies have low-quality evidence, so more high-quality research is needed.

Acknowledgement

This study was approved by the Ethics Committee of Isfahan University of Medical Sciences, Isfahan (approval number: IR.MUI.RESEARCH.REC.1399.603).

Conflict of Interest:

The authors declare that they have no conflict of interest.

References

  1. Lutz F, Krejci I. Resin composites in the post-amalgam age. Compendium of continuing education in dentistry Jamesburg. NJ 1995. 1999; 20: 1138-1148.
  2. Ritter AV, Walter R, Lee W. Sturdevant’s art and science of operative dentistry. North Carolina: Elsevier Health Sciences; 2019.
  3. Breschi L. Fundamentals of Operative Dentistry: A contemporary approach. Chicago: Quintessence Publishing; 2013.
  4. Murata T, Maseki T, Nara Y. Effect of immediate dentin sealing applications on bonding of CAD/CAM ceramic onlay restoration. Dent Mater J. 2018; 76: 928-939.
  5. Qanungo A, Aras MA, Chitre V, Mysore A, Amin B, Daswani SR. Immediate dentin sealing for indirect bonded restorations. J Prosthodont Res. 2016; 60: 240-249.
  6. Krämer N, Lohbauer U, Frankenberger R. Adhesive luting of indirect restorations. Am J Dent. 2000; 13: 60D-76D.
  7. Falkensammer F, Arnetzl GV, Wildburger A, Krall C, Freudenthaler J. Influence of different conditioning methods on immediate and delayed dentin sealing. J Prosthet Dent. 2014; 112: 204-210.
  8. Shakal MAS. Evaluation of zirconia-reinforced lithium silicate ceramic surface treatment on their shear bond strength to dentine following immediate dentin sealing. Egypt Dent J. 2017; 63: 3907-3913.
  9. Vinagre A, Ralho A, Ramos N, Messias A, Ramos J. Bonding performance of a universal adhesive: Effect of hydrophobic resin coating and long-term water storage. Rev Port Estomatol Med Dentária Cir Maxilofac. 2019; 60: 96-103.
  10. Rozan S, Takahashi R, Nikaido T, Tichy A, Tagami J. CAD/CAM-fabricated inlay restorations: Can the resin-coating technique improve bond strength and internal adaptation?. Dent Mater J. 2020; 39: 941-949.
  11. Pashley DH, Ciucchi B, Sano H, Horner JA. Permeability of dentin to adhesive agents. Quintessence Int. 1993; 24: 618-631.
  12. Magne P, Kim TH, Cascione D, Donovan TE. Immediate dentin sealing improves bond strength of indirect restorations. J Prosthet Dent. 2005; 94: 511-519.
  13. Rigos A, Dandoulaki C, Kontonasaki E, Kokoti M, Papadopoulou L, Koidis P. Effect of immediate dentin sealing on the bond strength of monolithic zirconia to human dentin. Oper Dent. 2019; 44: E167-E179.
  14. Hironaka NG, Ubaldini AL, Sato F, Giannini M, Terada RS, Pascotto RC. Influence of immediate dentin sealing and interim cementation on the adhesion of indirect restorations with dual-polymerizing resin cement. J Prosthet Dent. 2018; 119: 678.
  15. Choi YS, Cho IH. An effect of immediate dentin sealing on the shear bond strength of resin cement to porcelain restoration. J Adv Prosthodont. 2010; 2: 39.
  16. Hayashi K, Maeno M, Nara Y. Influence of immediate dentin sealing and temporary restoration on the bonding of CAD/CAM ceramic crown restoration. Dent Mater J. 2019; 38: 970-980.
  17. Dalby R, Ellakwa A, Millar B, Martin FE. Influence of immediate dentin sealing on the shear bond strength of pressed ceramic luted to dentin with self-etch resin cement. Int J Dent. 2012; 2012: 310702.
  18. Moher D, Liberati A, Tetzlaff J, Altman DG, PRISMA Group. Preferred reporting items for systematic reviews and meta-analyses: the PRISMA statement. Int J Surg. 2010; 8: 336-341.
  19. Sarkis-Onofre R, Skupien J, Cenci M, Moraes R, Pereira-Cenci T. The role of resin cement on bond strength of glass-fiber posts luted into root canals: a systematic review and meta-analysis of in vitro studies. Oper Dent. 2014; 39: E31-E44.
  20. Higgins JP, Thompson SG. Quantifying heterogeneity in a meta‐analysis. Stat Med. 2002; 21: 1539-1558.
  21. Ishii N, Maseki T, Nara Y. Bonding state of metal-free CAD/CAM onlay restoration after cyclic loading with and without immediate dentin sealing. Dent Mater J. 2017; 36: 357-367.
  22. Kitayama S, Pilecki P, Nasser NA, Bravis T, Wilson RF, Nikaido T, et al. Effect of resin coating on adhesion and microleakage of computer‐aided design/computer‐aided manufacturing fabricated all‐ceramic crowns after occlusal loading: a laboratory study. Eur J Oral Sci. 2009; 117: 454-462.
  23. Reboul T, Thaï HH, Cetik S, Atash R. Comparison between shear forces applied on the overlay-dental tissue interface using different bonding techniques: An in vitro study. J Indian Prosthodont Soc. 2018; 18: 212.
  24. Magne P. Immediate dentin sealing: a fundamental procedure for indirect bonded restorations. J Esthet Restor Dent. 2005; 17: 144-154.
  25. De Munck J, Vargas M, Iracki J, Van Landuyt K, Poitevin A, Lambrechts P, et al. One-day bonding effectiveness of new self-etch adhesives to bur-cut enamel and dentin. Oper Dent. 2005; 30: 39-49.
  26. Armstrong SR, Vargas MA, Fang Q, Laffoon JE. Microtensile bond strength of a total-etch 3-step, total-etch 2-step, self-etch 2-step, and a self-etch 1-step dentin bonding system through 15-month water storage. J Adhes Dent. 2003; 5: 47-56.
  27. Goracci C, Sadek FT, Monticelli F, Cardoso PE, Ferrari M. Influence of substrate, shape, and thickness on microtensile specimens’ structural integrity and their measured bond strengths. Dent Mater. 2004; 20: 643-654.
  28. Poitevin A, De Munck J, Van Landuyt K, Coutinho E, Peumans M, Lambrechtse P, et al. Critical analysis of the influence of different parameters on the microtensile bond strength of adhesives to dentin. J Adhes Dent. 2008; 10: 7-16.
  29. Pashley DH, Sano H, Ciucchi B, Yoshiyama M, Carvalho RM. Adhesion testing of dentin bonding agents: a review. Dent Mater. 1995; 11: 117-125.
  30. Gallusi G, Galeano P, Libonati A, Giuca MR, Campanella V. Evaluation of bond strength of different adhesive systems: Shear and Microtensile Bond Strength Test. Oral Implantol (Rome).. 2009; 2: 19.
  31. Takimoto M, Ishii R, Iino M, Shimizu Y, Tsujimoto A, Takamizawa T, et al. Influence of temporary cement contamination on the surface free energy and dentine bond strength of self-adhesive cements. J Dent. 2012; 40: 131-138.
  32. Ribeiro JC, Coelho PG, Janal MN, Silva NR, Monteiro AJ, Fernandes CA. The influence of temporary cements on dental adhesive systems for luting cementation. J Dent. 2011; 39: 255-262.
  33. Brigagão VC, Barreto LF, Gonçalves KA, Amaral M, Vitti RP, Neves AC, et al. Effect of interim cement application on bond strength between resin cements and dentin: Immediate and delayed dentin sealing. J Prosthet Dent. 2017; 117: 792-798.
  34. Papacchini F, Dall Oca S, Chieffi N, Goracci C, Sadek FT, Suh BI, et al. Composite-to-composite microtensile bond strength in the repair of a microfilled hybrid resin: effect of surface treatment and oxygen inhibition. J Adhes Dent. 2007; 9: 25.
  35. Pamato S, do Valle AL. Does hybridized dentin affect bond strength of self-adhesive resin cement?. J Clin Exp Dent. 2016; 8: e409.
  36. Seemann R, Flury S, Pfefferkorn F, Lussi A, Noack MJ. Restorative dentistry and restorative materials over the next 20 years: a Delphi survey. Dent Mater. 2014; 30: 442-448.
  37. Dietschi D, Monasevic M, Krejci I, Davidson C. Marginal and internal adaptation of class II restorations after immediate or delayed composite placement. J Dent. 2002; 30: 259-269.
  38. Irie M, Suzuki K, Watts D. Marginal gap formation of light-activated restorative materials: effects of immediate setting shrinkage and bond strength. Dent Mater. 2002; 18: 203-210.
  39. Cardenas AM, Siqueira F, Hass V, Malaquias P, Gutierrez MF, Reis A, et al. Effect of MDP-containing silane and adhesive used alone or in combination on the long-term bond strength and chemical interaction with lithium disilicate ceramics. J Adhes Dent. 2017; 19: 203-212.
  40. Pott PC, Stiesch M, Eisenburger M. Influence of 10-MD-P adhesive system on shear bond strength of zirconia-composite interfaces. Clin Oral Implants Res. 2015; 4: 117-126.
  41. Ito S, Hashimoto M, Wadgaonkar B, Svizero N, Carvalho RM, Yiu C, et al. Effects of resin hydrophilicity on water sorption and changes in modulus of elasticity. Biomaterials. 2005; 26: 6449-6459.
  42. Magne P. IDS: Immediate Dentin Sealing (IDS) for tooth preparations. J Adhes Dent. 2014; 16: 594.
  43. Malysa A, Wezgowiec J, Orzeszek S, Florjanski W, Zietek M, Wieckiewicz M. Effect of different surface treatment methods on bond strength of dental ceramics to dental hard tissues: A systematic review. Molecules. 2021; 26: 1223.
  44. Bona AD, Borba M, Benetti P, Cecchetti D. Effect of surface treatments on the bond strength of a zirconia-reinforced ceramic to composite resin. Braz Oral Res. 2007; 21: 10-15.
  45. Magne P, Douglas WH. Rationalization of esthetic restorative dentistry based on biomimetics. J Esthet Rest Dent. 1999; 11: 5-15.
  46. Magne P, Douglas WH. Porcelain veneers: Dentin bonding optimization and biomimetic recovery of the crown. Int J Prosthodont. 1999; 12: 111-121.
  47. Rueggeberg F, Margeson D. The effect of oxygen inhibition on an unfilled/filled composite system. J Dent Res. 1990; 69: 1652-1658.
  48. Khakiani MI, Kumar V, Pandya HV, Nathani TI, Verma P, Bhanushali NV. Effect of immediate dentin sealing on polymerization of elastomeric materials: an ex vivo randomized controlled trial. Int J Clin Pediatr Dent. 2019; 12: 288.
  49. Leesungbok R, Lee SM, Park SJ, Lee SW, Lee DY, Im BJ, et al. The effect of IDS (immediate dentin sealing) on dentin bond strength under various thermocycling periods. J Adv Prosthodont. 2015; 7: 224-232.
  50. Elbishari H, Elsubeihi ES, Alkhoujah T, Elsubeihi HE. Substantial in vitro and emerging clinical evidence supporting immediate dentin sealing. Jpn Dent Sci Rev. 2021; 57: 101-110.
  51. Magne P, Nielsen B. Interactions between impression materials and immediate dentin sealing. J Prosthet Dent. 2009; 102: 298-305.
  52. Gresnigt MM, Cune MS, Schuitemaker J, van der Made SA, Meisberger EW, Magne P, et al. Performance of ceramic laminate veneers with immediate dentine sealing: An 11 year prospective clinical trial. Dent Mater. 2019; 35: 1042-1052.
  53. Van den Breemer CR, Buijs GJ, Cune MS, Özcan M, Kerdijk W, Van der Made S, et al. Prospective clinical evaluation of 765 partial glass-ceramic posterior restorations luted using photo-polymerized resin composite in conjunction with immediate dentin sealing. Clin Oral Investig. 2021; 25: 1463-1473.